To address the challenges of brittle intermetallic compounds (IMCs), uneven microstructure, and high thermal stress concentration in laser welding of dissimilar steel and aluminum alloys, the work aims to investigate the effect of Si powder addition on the microstructure, phase evolution, and mechanical properties of laser welded TRIP steel/7075 aluminum alloy joints. The experiments were conducted via a fiber laser with deep-penetration lap welding, under varying welding speeds (10-16 mm/s) and laser powers (1 840-1 900 W). The joint quality was characterized by optical microscopy (OM), scanning electron microscopy (SEM), energy-dispersive X-ray spectroscopy (EDS), X-ray diffraction (XRD), electron backscatter diffraction (EBSD), and tensile-shear testing. The goal was to reveal the regulation mechanism of Si element on interfacial reactions and mechanical performance, thereby achieving a reliable steel-aluminum connection.
The results demonstrated that Si powder significantly improved weld appearance and process stability. The optimal parameters were determined as laser power 1 860 W, welding speed 14 mm/s, and defocusing distance +4 mm. Under these conditions, the weld was uniform, continuous, and free of obvious pores, spattering, or severe burn-through. Excessively low welding speed or high laser power caused overheating, large fusion width, voids, and interfacial cracks, whereas insufficient heat input led to incomplete fusion. The maximum tensile-shear force reached 2 328.2 N, increased by 53.2% compared with joints without Si powder, verifying the strengthening effect of the Si intermediate layer.
Microstructural analysis showed that Si addition modified the phase constituent at the steel-aluminum interface. Besides conventional Fe-Al binary IMCs such as FeAl, Fe2Al5, FeAl3, and Fe3Al, new Al-Fe-Si ternary phases including Al9Fe2Si2 and ductile Al0.5Fe3Si0.5 were formed. Si partially substituted Al or Fe in Fe-Al IMCs, suppressing the growth of thick and brittle Fe-Al layers. Consequently, the IMC thickness was remarkably reduced: 30.9 μm, 43.5 μm, and 28.2 μm at the left, right, and root interfaces, respectively, much thinner than approximately 46 μm in direct welding. Si also enhanced molten pool fluidity, promoting uniform mixing of Fe and Al, forming Al-enriched solute bands and Fe-enriched island zones.
EBSD results confirmed significant grain refinement and uniform microstructure. The average grain size at the interface was refined to 9.33 μm, decreased by 21.3% compared with that of Si-free joints. The Al-Fe-Si ternary phases distributed at grain boundaries exerted a strong pinning effect, inhibiting abnormal grain growth and enhancing grain size uniformity. These ternary phases acted as heterogeneous nucleation sites, increasing nucleation rate during solidification. Meanwhile, the proportion of low-angle grain boundaries was reduced to 1.79%, and the fraction of recrystallized structures reached 86.8%, which optimized residual stress distribution and improved joint toughness.
Fracture observations revealed a mixed fracture mechanism. The aluminum side exhibited intergranular brittle fracture with typical "rock-candy" morphology, while the steel side presented both cleavage steps and dimples, indicating a ductile-brittle hybrid mode. The formation of ductile Al0.5Fe3Si0.5 phase relieved local stress concentration and retarded crack propagation.
In conclusion, adding Si powder as an intermediate layer effectively regulates IMC phases, refines grains, optimizes grain boundary characteristics, and enhances the mechanical properties of laser welded TRIP steel/7075 aluminum alloy joints. This work provides a feasible, low-cost, and easily controlled method for joining steel and aluminum, supporting lightweight applications in automotive and aerospace manufacturing.
Key words
laser welding /
steel/aluminum joining /
Si powder intermediate layer /
microstructure /
mechanical properties
{{custom_sec.title}}
{{custom_sec.title}}
{{custom_sec.content}}
References
[1] LI T, WANG L X, QIU Z H, et al.Global Daily CO2 Emissions from 1970 to 2024[J]. Scientific Data, 2026, 13: 605.
[2] ESKANDER S M S U, FANKHAUSER S. Reduction in Greenhouse Gas Emissions from National Climate Legislation[J]. Nature Climate Change, 2020, 10(8): 750-756.
[3] WIMBADI R W, DJALANTE R.From Decarbonization to Low Carbon Development and Transition: A Systematic Literature Review of the Conceptualization of Moving Toward Net-Zero Carbon Dioxide Emission (1995- 2019)[J]. Journal of Cleaner Production, 2020, 256: 120307.
[4] 吴潇萌, 吴烨, 郝吉明. 我国汽车与环境协同发展进程中主要矛盾与发展方向研究[J]. 中国工程科学, 2018, 20(1): 74-83.
WU X M, WU Y, HAO J M.The Principal Contradiction and Coordination Development Strategies of Automobile Industry and Emission Control in China[J]. Strategic Study of CAE, 2018, 20(1): 74-83.
[5] 李晓瑜, 阎换丽, 程西西, 等. 新型铝合金材料在汽车轻量化中的应用[J]. 汽车电器, 2026(1): 134-136.
LI X Y, YAN H L, CHENG X X, et al.Application of New Aluminum Alloy Materials in Automotive Lightweighting[J]. Auto Electric Parts, 2026(1): 134-136.
[6] LI S H, ZHOU D S, PAN A X.Integrated Lightweight Optimization Design of Wall Thickness, Material, and Performance of Automobile Body Side Structure[J]. Structural and Multidisciplinary Optimization, 2024, 67(6): 95.
[7] 袁煜材, 吕国成. 新能源汽车节能与结构轻量化[M]. 北京: 机械工业出版社, 2020.
YUAN Y C, LYU G C.Energy Saving and Structural Lightweight of New Energy Vehicles[M]. Beijing: China Machine Press, 2020.
[8] 马鸣图, 王国栋, 王登峰, 等. 汽车轻量化导论[M]. 北京: 化学工业出版社, 2020.
MA M T, WANG G D, WANG D F.Introduction to Automotive Lightweight[M]. Beijing: Chemical Industry Press, 2020.
[9] XIA H B, TAO W, LI L Q, et al.Effect of Laser Beam Models on Laser Welding-Brazing Al to Steel[J]. Optics & Laser Technology, 2020, 122: 105845.
[10] 李岩, 胡志力, 于海洋, 等. 铝与钢异种材料连接技术及其研究进展[J]. 材料导报, 2020, 34(13): 13167-13174.
LI Y, HU Z L, YU H Y, et al.Research Progress and Technology of Dissimilar Joining between Aluminum and Steel[J]. Materials Reports, 2020, 34(13): 13167-13174.
[11] LI Q B, YANG S L, HU B G, et al.Laser Welding of Aluminum/Steel Dissimilar Metals and Control of Intermetallic Compounds: A Review[J]. The International Journal of Advanced Manufacturing Technology, 2025, 137(9): 4283-4308.
[12] 闫飞, 周一凡, 唐本刊, 等. 铝钢异种材料激光搭接焊接头组织与性能研究[J]. 应用激光, 2023, 43(2): 65-69.
YAN F, ZHOU Y F, TANG B K, et al.Microstructure and Mechanical Properties of Aluminum/Steel Dissimilar Laser Lap Welding Joints[J]. Applied Laser, 2023, 43(2): 65-69.
[13] YUCE C, KARPAT F, YAVUZ N.Investigations on the Microstructure and Mechanical Properties of Laser Welded Dissimilar Galvanized Steel-Aluminum Joints[J]. The International Journal of Advanced Manufacturing Technology, 2019, 104(5): 2693-2704.
[14] FAN J, THOMY C, VOLLERTSEN F.Effect of Thermal Cycle on the Formation of Intermetallic Compounds in Laser Welding of Aluminum-Steel Overlap Joints[J]. Physics Procedia, 2011, 12: 134-141.
[15] SZCZEPANIAK A, FAN J F, KOSTKA A, et al.On the Correlation between Thermal Cycle and Formation of Intermetallic Phases at the Interface of Laser-Welded Aluminum-Steel Overlap Joints[J]. Advanced Engineering Materials, 2012, 14(7): 464-472.
[16] MA J J, HAROONI M, CARLSON B, et al.Dissimilar Joining of Galvanized High-Strength Steel to Aluminum Alloy in a Zero-Gap Lap Joint Configuration by Two-Pass Laser Welding[J]. Materials & Design, 2014, 58: 390-401.
[17] LI T, ZHOU D W, YAN Y, et al.Effect of Ti Foil on Microstructure and Mechanical Properties of Laser Fusion Welding of DP590 Dual-Phase Steel to 6022 Aluminum Alloy[J]. Materials Science and Engineering: A, 2020, 796: 139929.
[18] XU T Y, ZHOU S W, WU H, et al.Effect of Nickel Interlayer Thickness on Lap Joint Laser Welding for Aluminium-Steel Dissimilar Materials[J]. Science and Technology of Welding and Joining, 2022, 27(3): 166-175.
[19] 周惦武, 刘元利, 李宁宁, 等. 添加Sn-5%Zr粉末对激光焊接钢/铝显微组织和性能影响[J]. 中国激光, 2015, 42(5): 87-95.
ZHOU D W, LIU Y L, LI N N, et al.Effect of Sn-5%Zr Powder Addition on Microstructure and Mechanical Property of Steel/Al Laser Welding[J]. Chinese Journal of Lasers, 2015, 42(5): 87-95.
[20] LONG J Q, HUANG W H, XIANG J W, et al.Parameter Optimization of Laser Welding of Steel to Al with Pre- Placed Metal Powders Using the Taguchi-Response Surface Method[J]. Optics & Laser Technology, 2018, 108: 97-106.
[21] RAHMAN S A A, MAMAT S, AHMAD M I, et al. Study on Intermetallic Compound (IMC) in Dissimilar Joining of Steel and Aluminum (Fe-Al): A Review Paper[J]. Welding in the World, 2024, 68(9): 2351-2376.
[22] LI B L, ZHOU J Y, PAN H, et al.Control of the Intermetallic Compound of the Laser Welding-Brazing Steel- Al Joint and Its Effect on the Joint Property[J]. Journal of Materials Research and Technology, 2025, 36: 2839-2848.
[23] WANG H H, MENG L, LUO Q, et al.Superior Cryogenic Toughness of High-Mn Austenitic Steel by Welding Thermal Cycles: The Role of Grain Boundary Evolution[J]. Materials Science and Engineering: A, 2020, 788: 139573.
[24] AN X H, WU S D, ZHANG Z F, et al.Enhanced Strength-Ductility Synergy in Nanostructured Cu and Cu-Al Alloys Processed by High-Pressure Torsion and Subsequent Annealing[J]. Scripta Materialia, 2012, 66(5): 227-230.
[25] WANG Y M, CHEN M W, ZHOU F H, et al.High Tensile Ductility in a Nanostructured Metal[J]. Nature, 2002, 419(6910): 912-915.
Funding
Jilin Provincial Science and Technology Development Program Project (20230201108GX)