目的 为探究热处理对超音速等离子喷涂铁基非晶涂层结构演化及耐磨性能的影响规律,明确结构弛豫与晶化转变对磨损行为的调控机制。方法 采用超音速等离子喷涂技术制备铁基非晶涂层,并在300、500、700 ℃条件下进行热处理。通过差示扫描量热分析确定涂层晶化温度,利用X射线衍射和扫描电子显微镜表征涂层结构及微观形貌演化,并结合显微硬度测试、纳米压痕测试及球-盘式摩擦磨损试验系统评价其力学性能与耐磨性能变化。结果 涂层起始晶化温度约为650 ℃。随着热处理温度升高,涂层由非晶态逐渐向晶态转变,其中300 ℃时主要发生结构弛豫,500 ℃出现初始晶化特征,而700 ℃则发生明显晶化,并形成α-Fe及Fe-Cr晶相。适度热处理显著降低了涂层孔隙率并提高致密性和显微硬度,其中500 ℃热处理后涂层具有最高的H/E及H3/E2值,表现出更优异的抗接触损伤能力和最佳耐磨性能;而700 ℃热处理导致孔隙率回升并引入裂纹等缺陷,涂层耐磨性能明显下降。磨损形貌分析表明,涂层磨损机制由喷涂态及低温条件下的磨粒磨损逐渐转变为高温条件下以磨粒磨损与剥落磨损共同作用。结论 热处理通过调控铁基非晶涂层的结构状态及缺陷分布,显著影响其力学性能与磨损行为。适度结构弛豫有助于提升涂层致密性、承载能力及抗接触损伤能力,从而改善耐磨性能,而过度晶化则导致脆性增加及结构不稳定性增强,是引起磨损加剧的主要原因。
Abstract
The work aims to clarify the effect of heat treatment on the microstructural evolution and tribological properties of Fe-based amorphous coatings prepared by supersonic plasma spraying, with particular emphasis on the roles of microstructural relaxation and crystallization in governing wear behavior.
Fe-based amorphous coatings were deposited via a supersonic plasma spraying system under optimized processing conditions. Post-deposition heat treatments were conducted at 300 ℃, 500 ℃, and 700 ℃ to induce different microstructural states. Differential scanning calorimetry was employed to determine the crystallization temperature of the as-sprayed coating. The phase microstructure evolution was characterized by X-ray diffraction and the microstructural features, including porosity and defect distribution, were analyzed through scanning electron microscopy. Microhardness and nanoindentation testing were performed to evaluate the mechanical response, and ball-on-disk tribological tests were carried out to assess friction and wear performance. The wear mechanisms were further analyzed based on worn surface morphologies.
The results reveal that the crystallization temperature of the coating is approximately 650 ℃. With the increasing heat treatment temperature, the coating undergoes a progressive transition from an amorphous microstructure to a crystalline state. At 300 ℃, microstructural relaxation dominates, leading to a reduction in free volume and porosity, and resulting in a denser microstructure. The porosity decreases from (6.76±0.52)% in the as-sprayed state to (4.98±0.41)%, accompanied by an increase in microhardness and improved load-bearing capacity. Consequently, the friction coefficient decreases and the wear loss is minimized. At 500 ℃, the coating exhibits initial crystallization characteristics together with the highest H/E and H3/E2 values, indicating superior resistance to contact damage and optimal wear resistance. The porosity further decreases to approximately (4.02±0.36)%. However, the associated volume changes and stress redistribution induce localized microcracks, which negatively affects microstructural stability and leads to increased fluctuations in friction behavior. At 700 ℃, significant crystallization takes place, accompanied by the formation of α-Fe and Fe-Cr crystalline phases, while the amorphous diffraction hump is markedly weakened. This results in a deterioration of mechanical integrity, including increased brittleness, crack propagation, and a slight increase in porosity to approximately (4.65±0.47)%. As a result, both friction coefficient and wear loss increase markedly. The wear mechanism evolves correspondingly with microstructural changes. The as-sprayed and low-temperature- treated coatings are dominated by mild abrasive wear due to improved surface integrity and stability. In contrast, coatings treated at higher temperatures exhibit a combination of abrasive wear and delamination wear, driven by crack initiation, propagation, and material spallation. Detached debris further aggravates abrasive interactions at the contact interface.
Overall, this work demonstrates that heat treatment serves as an effective approach to tailor the microstructure and tribological properties of Fe-based amorphous coatings. Moderate heat treatment enhances coating densification, load-bearing capacity, and resistance to contact damage through microstructural relaxation, while excessive crystallization deteriorates coating performance due to increased brittleness and defect formation. These findings provide useful insights into the optimization of amorphous coatings for wear-resistant applications.
关键词
铁基非晶涂层 /
热处理 /
结构演化 /
摩擦磨损
Key words
Fe-based amorphous coating /
heat treatment /
microstructural evolution /
tribological wear
{{custom_sec.title}}
{{custom_sec.title}}
{{custom_sec.content}}
参考文献
[1] 袁大鹏, 杨文安, 南健, 等. 超音速火焰喷涂制备铁基非晶涂层工艺[J]. 粉末冶金工业, 2025, 35(6): 51-56.
YUAN D P, YANG W A, NAN J, et al.The Process of Iron-Based Amorphous Coating Prepared by High- Velocity Oxygen-Fuel[J]. Powder Metallurgy Industry, 2025, 35(6): 51-56.
[2] GAO T Z, GAO J, ZHOU H, et al.Achieving Superior Corrosion Resistance in HVAF-Sprayed Fe-Based Amorphous Alloy Coatings through Data-Driven Machine Learning[J]. Journal of Materials Science & Technology, 2026, 247: 171-187.
[3] 王一凡, 谢心怡, 郝钰宁, 等. TiZrHfCuBe高熵非晶合金室温压痕蠕变行为[J]. 金属功能材料, 2025, 32(1): 82-86.
WANG Y F, XIE X Y, HAO Y N, et al.Room Temperature Indentation Creep Behavior of TiZrHfCuBe High-Entropy Metallic Glass[J]. Metallic Functional Materials, 2025, 32(1): 82-86.
[4] 罗锐恒, 智小琦, 张姚瑶. Zr基非晶合金反应材料的力学性能与冲击烧蚀特性[J]. 金属功能材料, 2023, 30(3): 83-92.
LUO R H, ZHI X Q, ZHANG Y Y.Mechanical Properties and Impact Ablation Characteristics of Zr-Based Amorphous Alloy Reactive Materials[J]. Metallic Functional Materials, 2023, 30(3): 83-92.
[5] YANG Z L, ZHENG A D, LI X Y, et al.Process Exploration for Superhydrophobic Surface Formation on Fe-Based Amorphous Alloys via Selective Laser Melting[J]. Applied Surface Science, 2026, 730: 166277.
[6] 宋培松, 张志彬, 邵里良, 等. 热输入对等离子喷涂(FeCoCrNi)75B15Si10高熵非晶合金涂层耐磨损性能的影响[J]. 中国表面工程, 2026, 39(1): 74-83.
SONG P S, ZHANG Z B, SHAO L L, et al.Effect of Heat Input on the Wear Resistance of (FeCoCrNi)75B15Si10 High-Entropy Amorphous Alloy Coatings Prepared Using Plasma Spraying[J]. China Surface Engineering, 2026, 39(1): 74-83.
[7] SONG Y, JIN G, MA G Z, et al.The Tribological Behavior Differences of Supersonic Atmospheric Plasma Sprayed Nanocrystalline Al-Si-Ce and Al-Si-Ce-Y Coatings at Room Temperature and 210 ℃[J]. Tribology International, 2026, 216: 111521.
[8] HE G C, GUO W L, ZHOU L L, et al.Thermal Control of Supersonic Atmospheric Plasma Spraying Al2O3-Based Coatings Doped with MgO[J]. Ceramics International, 2026, 52(7): 9203-9216.
[9] LV J S, LI W, LI T, et al.Ablation Behavior of High-Entropy Boride (Hf-Zr-Ta-Ti)B2 Coating Fabricated via Supersonic Atmospheric Plasma Spraying for Carbon/Carbon Composites[J]. Composites Part B: Engineering, 2024, 270: 111137.
[10] CHEN S, HE D X, ZHU Y L, et al.Research on the Ablation Damage Evolution of Al2O3/PF Composite Coatings Deposited by Supersonic Plasma Spraying on Resin Matrix Surfaces[J]. Surface and Coatings Technology, 2025, 513: 132463.
[11] YE Y Z, GUO Z J, ZHOU Z J, et al.Improved Corrosion and Corrosion-Wear Properties of Fe-Based High-Entropy Amorphous Coatings by Modulating Heat Input of HVAF[J]. Corrosion Science, 2024, 232: 112049.
[12] WU L T, LAN T R, WANG G Y, et al.Thermal Treatment-Induced Structural Homogenization and Multifunctional Performance Enhancement in TiNx-Reinforced Amorphous Composite Coatings[J]. Surface and Coatings Technology, 2026, 520: 133067.
[13] 高鹏飞, 陈永君, 王增睿, 等. 铁基非晶涂层的研究进展与应用[J]. 表面技术, 2023, 52(3): 64-74.
GAO P F, CHEN Y J, WANG Z R, et al.Research Progress and Application of Fe-Based Amorphous Coatings[J]. Surface Technology, 2023, 52(3): 64-74.
[14] YAN S, YUAN J C, MA C, et al.Innovative Preparation and Corrosion Resistance of Fe-Based Amorphous Coatings Fabricated by Ultra Short Pulse Laser Manufacturing Process[J]. Journal of Alloys and Compounds, 2025, 1049: 185410.
[15] 朱帅帅, 张保森, 孙然, 等. 热处理对HVAF喷涂CoNiCrMo基高熵非晶涂层结构与摩擦学性能的影响[J]. 中国表面工程, 2026, 39(1): 119-130.
ZHU S S, ZHANG B S, SUN R, et al.Effects of Heat-Treatment on the Microstructure and Tribological Properties of CoNiCrMo-Based High Entropy Amorphous Alloy Coating Sprayed by HVAF[J]. China Surface Engineering, 2026, 39(1): 119-130.
[16] 张香云, 丁国强, 袁子洲. 热处理对冷喷涂铁基非晶涂层耐腐蚀性能的影响[J]. 金属热处理, 2025, 50(3): 270-276.
ZHANG X Y, DING G Q, YUAN Z Z.Influence of Heat Treatment on Corrosion Resistance of Cold-Sprayed Fe-Based Amorphous Coatings[J]. Heat Treatment of Metals, 2025, 50(3): 270-276.
[17] JIANG M F, WANG J J, CAI M J, et al.Improvement of Soft Magnetic Properties for Fe-Based Amorphous/Nanocrystalline Alloy by Longitudinal Magnetic Field Annealing[J]. Journal of Non-Crystalline Solids, 2025, 650: 123382.
[18] 李广, 王小东, 张晶, 等. 电热爆炸沉积Fe基非晶涂层结构对性能的影响[J]. 表面技术, 2025, 54(18): 77-85.
LI G, WANG X D, ZHANG J, et al.Effects of Structure on Properties of Fe-Based Amorphous Coatings Prepared by Electrothermal Explosion[J]. Surface Technology, 2025, 54(18): 77-85.
[19] HUANG F, KANG J J, YUE W, et al.Effect of Heat Treatment on Erosion-Corrosion of Fe-Based Amorphous Alloy Coating under Slurry Impingement[J]. Journal of Alloys and Compounds, 2020, 820: 153132.
[20] 王贺千, 康嘉杰, 王浩东, 等. 铁基非晶合金涂层的制备及其耐磨防腐性能研究进展[J]. 材料工程, 2025, 53(2): 1-13.
WANG H Q, KANG J J, WANG H D, et al.Research Progress in Preparation and Wear Corrosion Resistance of Fe-Based Amorphous Alloy Coatings[J]. Journal of Materials Engineering, 2025, 53(2): 1-13.
[21] 景瑞, 俞伟元, 王明康. 爆炸喷涂氧燃比对铁基非晶涂层性能的影响[J]. 电焊机, 2026, 56(2): 73-82.
JING R, YU W Y, WANG M K.Effect of Oxygen to Fuel Ratio by Explosive Spraying on Properties of Iron-Based Amorphous Coatings[J]. Electric Welding Machine, 2026, 56(2): 73-82.
[22] ZHANG K C, LIU X, HE Y, et al.Unveiling the Impact of Hydrogen Permeation on the Nanoindentation Creep Behavior of Plasma-Sprayed Fe-Based Amorphous Coatings[J]. Intermetallics, 2026, 188: 109057.
[23] 王红哲, 杨德明, 赵中杰, 等. 基体温度对等离子喷涂铁基非晶合金涂层耐磨耐蚀性的影响[J]. 表面技术, 2024, 53(19): 201-211.
WANG H Z, YANG D M, ZHAO Z J, et al.Effect of Substrate Temperature on Wear and Corrosion Resistance of Plasma Sprayed Iron-Based Amorphous Coatings[J]. Surface Technology, 2024, 53(19): 201-211.
[24] HALDER S, FARIDI M A, ROUT A, et al.Optimization of Wetting Behavior in Plasma-Sprayed Fe-Based Amorphous/Crystalline Coatings Resulting Improved Corrosion Inhibition Ability[J]. Surface and Coatings Technology, 2025, 495: 131562.
[25] ZUO J D, LI J, WANG J N, et al.Balancing the Strength-Plasticity Dilemma via Hierarchical Interfaces in Crystalline Cr/Amorphous CrAlN Nanolaminates[J]. Journal of Materials Science & Technology, 2026, 245: 266-277.
[26] GAO Z G, YUAN S Q, HOU X, et al.Nanostructured Crystalline-Amorphous FeCrCoNi-SiC High-Entropy Alloy Thin Film with a Superior Combination of Strength and Corrosion Resistance[J]. Applied Surface Science, 2025, 685: 162091.
[27] 龚伟莹, 周志丹, 张永振, 等. 铁基非晶涂层的制备及耐磨耐蚀性的研究进展[J]. 热加工工艺, 2025, 54(18): 21-26.
GONG W Y, ZHOU Z D, ZHANG Y Z, et al.Research Progress on Preparation and Wear and Corrosion Resistance of Fe-Based Amorphous Coatings[J]. Hot Working Technology, 2025, 54(18): 21-26.
[28] ZOU G P, QI Y X, WANG Q Q, et al.Enhanced Anti-Wear Properties of HVOF-Sprayed Fe-Cr-Mo-C-B High-Entropy Amorphous Composite Coatings via Heat Input Modulation[J]. Tribology International, 2026, 219: 111848.
[29] 李旭强, 李文生, 翟海民, 等. Fe基非晶涂层厚度与其爆炸喷涂沉积特性及性能[J]. 表面技术, 2023, 52(5): 140-148.
LI X Q, LI W S, ZHAI H M, et al.Effect of Coating Thickness on Fe-Based Amorphous Detonation Spraying Deposition Characteristics and Properties[J]. Surface Technology, 2023, 52(5): 140-148.
[30] 胡明超, 赵运才, 王慧鹏, 等. 铁基非晶涂层的研究现状及应用[J]. 中国表面工程, 2025, 38(4): 179-197.
HU M C, ZHAO Y C, WANG H P, et al.Research Status and Application of Fe-Based Amorphous Coatings[J]. China Surface Engineering, 2025, 38(4): 179-197.